Dear Experts I never woarked with Mat. thk. less than 6mm. I dont the code with me. Now we have to qualify PQR for welding SS316L HVAC Ducts ( thk 3mm ) Prefer to use SMAW, FCAW or GTAW Appreciate you share your experience:-
1) Thk Range Qualified 2) Mechanical Test Redq 3) Challenges in qualifying PQR and on production welding 4) Welder Qualification 5) Prefer to use KOBELCO or ESAB consumables 6) Essential and Non-Essential Varibales for PQR & WQT qualifcations
I agree with Lawrence. We have always used AWS D9.1 for HVAC ducts with GMAW-Short circuiting or GTAW process. As I recall, a 4G test with 10 ga. and 18 ga. coupons qualifies all positions and sheet metal gage thicknesses.
As Al Moore points out, D 1.6 covers welding the sheet thicknesses of Stainless Steel. If D 1.1 was specified in your contract, it may be necessary to work to D 1.6 "by reference". However, if you can get away with it, D 9.1 is the way to go.