- - By Nalla (***) Date 06-09-2010 21:39
Welder qualified using SMAW and F4 ( E7016) Electrodes.
Is he also qualified to weld with F5 Electrode to Stainless Steel ( Butt or Fillet Welds )?
All I know When F5 group of elctrodes used for welder qualification , he only  qualified for F5 & F1 ( SFA 5.5).
I'm confused with QW-404-14( Essential Variable for Welding Consumable limitations and QW-420(Wide range of base material qualified to weld )
If he is qualified, in ref to which sect?
Pls advise, Thanks
Parent - By Shane Feder (****) Date 06-10-2010 00:05
Nalla,
QW 433
F4 with backing qualifies for F 1, 2, 3 & 4 with backing
F 4 without backing qualifies for F 4 without backing and F 1, 2, 3 & 4 with backing
Hope that helps,
Regards,
Shane