- - By Toey TNDT (**) Date 02-12-2014 09:46
Dear Sir ,

IN EN15614-1 7.4.5 IMPACT TESTING
IF MY PROCESS IS GTAW+SMAW MATERIAL IS SA335 P11
I HAVE TO TEST ABOUT 12 EA. OR NOT ?

IN GTAW 3 EA , SMAW 3 EA , HAZ GTAW P11 3 EA , HAZ SMAW 3 EA OR JUST HAZ 3 EA

PLEASE CLARIFY ME

THANK YOU FOR ADVANCE

TOEY_TNDT
Parent - By nantong (**) Date 02-15-2014 13:13
Two sets of three required. Weld metal and HAZ 2mm below the surface unless material is greater than 50mm thick where an additional two sets are required weld and HAZ either mid-thickness or root. GTAW and SMAW has no relevance it is only weld metal.