- - By dragon (**) Date 08-30-2004 23:25
15NiCuMoNb5 (WB36) What electroce match?

How about ER80S-G/E9018-G ?
Parent - - By R-win (*) Date 08-31-2004 07:02
All designations "-G" means in principle "not specified". Only tensile strength is specified.
For WB36 often the 0,5%Mo TIG rods can be taken for root and fil with 1%Ni-and 0,3-0,5%Mo. Also depending on required charpy values (at -40°C?). PHOENIX SH Schwarz 3 K Ni (SMAW). UNION S3NiMo1 with UV 420TT(R) or UV421TT (SAW). Böhler DMO-IG (GTAW).
Parent - By dragon (**) Date 09-15-2004 11:47
15NiCuMoNb/A106B should fill what materal?
Parent - By MBSims (****) Date 09-16-2004 00:09
I'm not familiar with that material, but did find a WPS that uses the following filler:

Böhler DMO-IG / Böhler FOX DMO Kb 2.50/250 / Böhler FOX DMO Kb 3.25/350