Sourdough,
(please don't take offense, several of my guys didn't understand why I get on them about the arc strikes outside of the weld joint until they took part in this test that I'm about to tell you about)
Let me show you a couple picts of an arc strike, and you may understand why the guys are riding you about your comment. I took several pieces of regualr ole A36 flatbar 3/8" thick and laid them on a table side by side an had one of my welders take a 7018 and drag it quickly across them, then had them look at them and grind the strike out until they felt the damage was no longer there. Then I took those same pieces of flatbar and bent them in my weld coupon bender and here is what happened....
Note: the first piece of flatbar was arc strike free, the rest were laid side by side and had a 7018 drug across them, and then ground.

and here is a close up (used the camera here at work so the quality isn't the best)