That figure is one of the weldor tests you can give, just make sure its the one you really need. (I personally have not done a 3/8" test plate in over 10 years, a total waist of my time, do it with 1/2" or more. Side bends are easy, with less prep to do the bends)
The Short Version:
Start with table 4.10 find the joints your weldor is going to doing, then go to table 4.11 find your joint covering the most or all being used in production, (note the thickness) this table lists all the test parameters/ranges along with the figure that goes with each test. If you don't already have a WPS for testing, write one around the process, electrode manufactures recommendations, amp/volt range that works etc. etc. etc......................... Assuming you have access to the test equipment to finish the test you are giving you can now finish the test. Note Part C - 4.18.3 will take you to 4.8.1 for visual, and don't forget 4.22, this is the most missed part of a WQTR document, see sample Form N-4.
For Prequalified joints as used in production go to Clause 3, Clause 4 is for qualification testing of PQRs. WPSs. WQTRs only. (except table 4.5 is referred to in Clause 3.6)
I posted this the other day and it may be of help to you also. I listed the code references that go along with the requested information on the documentation. Its from the 04
Enjoy
Type of Weldor (D1.1.4.1.2)(Manual or Machine)
Variables (D1.14 Part C.4.7 & 4.21 & 4.22 Table 4.11)(D1.5.5.24)
Material / Specification (D1.1 Table 3.1)(D1.5.5.21.3) To
Base Metal (D1.1.3.3)(D1.1.1.2 - 100 ksi yield limit)(D1.5.5.24.1.1 - 90 ksi yield limit)(D1.5.1.2.2 & 5.4.3 base metals)
Plate Thickness: (D1.1 Table 4.10)(D1.5 Table 5.7)
Groove: (D1.1.3.7.2)(D1.1.4.23 & 4.30)(D1.5.5.23.1.2)
Fillet: (D1.1.3.7.2)(D1.1.4.25 & 4.30)(D1.5.5.23.1.3)
Pipe Diameter / Thickness: (D1.1 Table 4.10)
Groove: (D1.1.4.26 & 4.30)
Fillet: (D1.1.4.30)
Joint Type (D1.1.3.9, 3.10, 3.11, 3.12 & 3.13)(D1.1 Table 3.7 & Figures 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 3.10 &3.11)
Process / Type (D1.1.3.2.3)(D1.1.Table 4.11 #1)(D1.5.5.24.1.2)
Backing (D1.1.4.19.1.2)(D1.1.Table 4.11 #6)(D1.5.5.23.1.2 & 5.24)___________Size (D1.1.5.10.3)(D1.5.3.13.4) __________
Position (D1.1.4.23.1 Table 4.9)(D1.5.5.24.2.2)
Weld Progression (D1.1.3.7.1)(D1.5.4 .6.8)
Filler Metal (D1.1.3.3)(D1.1.Table 4.11-Item 3)(D1.1.5.3.2.2)(D1.5 Tables 4.1, 4.2 & 4.3)
Specification No. / Class (D1.1.Table 3.1)(B2.1 Table C1)
F Number (D1.1.Table 4.11-Item 2 & Table 4.12)(B2.1 Table C1)
Gas / Flux Type (D1.1.Table 4.11-Note 2)(D1.1.4.22)(D1.5 Table 5.3 #13)__________ Flow Rate _____________
Electrode (D1.1.5.3.4)(D1.1.5.3.2, 5.3.2.1)(D1.5.5.24.2.1)
Single / Multiple (D1.1 Table 3.7)(D1.1.Table 4.5 #11 & 4.11 #7)(D1.5.5.21.2)
Diameter / Manufacturer (D1.1 Table 3.7) (D1.1.5.3.3.1)(D1.1.Table 4.5 #10)(D1.5.5.21.2)
Welding Procedure Specification No. (D1.1 Table 3.7)(D1.1.5.5)(D1.5.5.21.2)(D1.1.3.6) Rev.
Preheat (D1.1.3.5)(D1.1.5.6 & 5.7)(D1.5.4.2) Maximum Interpass Temperature
Stringer or Weave (D1.1.Table 4.6 #11)(D1.5.5.12 & 5.13 & Table 5.3)(see KJ inch heat input)
Current / Polarity (D1.1.3.6 Table 3.7)(D1.5.21.2) Volts ___________Amps____________ + or -Polarity_______
Travel Speed________ Rod Temperature (D1.1.5.3.2.2) (D1.5.4.5) __________CVN _________ F° ________ lbs
Minimum required KJ inch (D1.1.Table 4.5 & 4.6)(D1.5.5.12, 5.13 Tables 5.3, 12.3, 12.4 & 12.5)
(Volts x Amps x .06 divided by Travel speed = KJ inch) or (Volts x Amps x .06 divided by KJ inch = Travel speed)
Weldor Test Information (D1.1 Annex E Form E-4)(D1.5 Annex III Form III-4)
Name _________ ID # _________
Type of Weldor (D1.1.4.1.2)__________ Date of Test ____________
Welding Procedure Specification No. (D1.1 Table 3.7)(D1.1.5.5)(D1.5.5.21.2)(D1.1.3.6) Rev.
Variables (D1.14 Part C.4.7 & 4.21 & 4.22 Table 4.11)(D1.5.5.24) Record actual values used in qualification test
Process / Type (D1.1.3.2.3)(D1.1.Table 4.11 #1)(D1.5.5.24.1.2)
Stringer or Weave (D1.1.Table 4.6 #11)(D1.5.5.12 & 5.13 & Table 5.3)
Current / Polarity (D1.1.3.6 Table 3.7)(D1.5.21.2) Volts_____ Amps_______ + or - polarity _______
Position (D1.1.4.23.1 Table 4.9)(D1.5.5.24.2.2)
Weld Progression (D1.1.3.7.1)(D1.5.4 .6.8)
Backing (D1.1.4.19.1.2)(D1.1.Table 4.11 #6)(D1.5.5.23.1.2 & 5.24) __________Size (D1.1.5.10.3)(D1.5.3.13.4)__________
Material / Specification (D1.1 Table 3.1)(D1.5.5.21.3)__________To____________Heat #_____________
Joint Type (D1.1.3.9, 3.10, 3.11, 3.12 & 3.13)(D1.1 Table 3.7 & Figures 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 3.10 &3.11)
Electrode (D1.1.5.3.4)(D1.1.5.3.2, 5.3.2.1)(D1.5.5.24.2.1)
Single / Multiple (D1.1 Table 3.7)(D1.1.Table 4.5 #11 & 4.11 #7)(D1.5.5.21.2)
Diameter / Manufacturer (D1.1 Table 3.7)(D1.1.Table 4.5 #10)(D1.5.5.21.2)
Filler Metal (D1.1.3.3)(D1.1.3.3)(D1.1.Table 4.11-Item 3)(D1.1.5.3.2.2)(D1.5 Tables 4.1, 4.2 & 4.3)
Specification No. / Class (D1.1.Table 3.1)(B2.1 Table C1)
F Number (D1.1.Table 4.11-Item 2 & Table 4.12)(B2.1 Table C1)
Gas / Flux Type (D1.1.Table 4.11-Note 2)(D1.1.4.22)(D1.5 Table 5.3 #13)_________ Flow Rate_________
Base Metal (D1.1.3.3)(D1.1.1.2 - 100 ksi yield limit)(D1.5.5.24.1.1 - 90 ksi yield limit)(D1.5.1.2.2 & 5.4.3 base metals)
Plate Thickness: (D1.1 Table 4.10)(D1.5 Table 5.7)
Groove: (D1.1.3.7.2)(D1.1.4.23 & 4.30)(D1.5.5.23.1.2)
Fillet: (D1.1.3.7.2)(D1.1.4.25 & 4.30)(D1.5.5.23.1.3)
Pipe Diameter / Thickness: (D1.1 Table 4.10)
Groove: (D1.1.4.26 & 4.30)
Fillet: (D1.1.4.30)
Rod Temperature (D1.1.5.3.2.2) (D1.5.4.5)_________Wind (D1.1.5.12.1)(D1.5.4.14.3)________
Preheat (D1.1.3.5)(D1.1.5.6 & 5.7)(D1.5.4.2)_______ Maximum Interpass Temperature________
Ambient Temperature (D1.1.5.12.2)(D1.5.4.2)_______Weld Length______ Travel Speed__________
Minimum required KJ inch (D1.1.Table 4.5 & 4.6)(D1.5.5.12, 5.13 Tables 5.3, 12.3, 12.4 & 12.5)
(Volts x Amps x .06 divided by Travel speed = KJ inch) or (Volts x Amps x .06 divided by KJ inch = Travel speed)
Appearance of welds (D1.1.4.8.1)(D1.5.6.26)(D1.5.5.21.5)(D1.5.6.4.4 Inspector observation required)
Root pass (D1.1.4.8.1-4&5)(D1.1 Table 6.1)(D1.5.6.26.1.2)(D1.5.5.21.5)
Intermediate passes (D1.1 Table 6.1)(D1.1.5.30)(D1.5.6.26.1.2)(D1.5.3.11)(D1.5.5.21.5)
Cover pass (D1.1.4.8.1)(D1.1 Table 6.1)(D1.1.5.24, 5.27 & 5.28)(D1.5.3.6, 3.8 & 3.9)(D1.5.6.26)
Undercut (D1.1.4.8.1)(D1.5.5.27.1)
Porosity (D1.1 Table 6.1)(D1.5.5.27.4.1)(D1.5.6.26.1.6)
Arc Strikes (D1.1.5.29)(D1.5.3.10)
Name of Welding Test Witness (D1.5.6.4.4 Inspector observation required)