Up Topic American Welding Society Services / Technical Standards & Publications / AWS D1.1-Single V PQR for Double Bevel Joint
- - By Nalla (***) Date 10-21-2010 22:18
Dear Friends
AWSD1.1-Table 4.6
Existing PQR - Base Material - EH36 x 25.4 / Weld Process - SMAW / Weld Position - 3G / Charpy: -40 deg celcius qualified.
Can I use this PQR to weld double bevel T-Joints? ( Base Material - EH36 X 383mm thk / Weld Process - SMAW / Weld Positions - 1G , 2G & 3G involved )
Appreciate expert guidance
Thanks
Parent - - By 803056 (*****) Date 10-22-2010 12:50
It would depend on the material thickness, the size of the welds, positions, whether you can meet prequalification requirements or not.

Al
Parent - - By Nalla (***) Date 10-22-2010 21:40
Dear Friends
It is Double Bevel T-FP crane column(38mm thk x EH36) connection Side Shell(19mm thk x EH36)
Weld PositionS - 3G & 4G / Weld Process - SMAW
Thanks
Parent - By 803056 (*****) Date 10-23-2010 04:41
If by EH36, you are referring to ABS EH36, it is a prequalified base metal. Provided you meet the other conditions of prequalification as delineated by Clause 3 of D1.1, you should be ready to weld once you write a prequalified WPS.

Best regards - Al