It's been nearly 25 years since I've last worked on ground-engauging equipment (bucket teeth, ripper shanks,ect). Any ideas for a refresher course on high carbon and manganese weldments? The memory dims as time passes. Ed
Thanks, found some good reading. I'm more interested in applicable pre-heat temps, interpass temps, and what new products may be available for manganese steel. I remember some names like 'stoody' and 'hastaloy', but that was a while back.
You should be using a stainless steel alloy which is close to 18 Cr, 8 Ni and 5 Mn. For eg. Citochromax N of Oerlikon.
The above composition suits best to joint manganese steel. it has some work hardening property as well.
The rules of the game are :
1. Before welding, ensure that the parts are in the quenched (softened) state. It would be a bad idea to weld manganese steel which is already work hardened to some extent. 2. Do not preheat. 3. Keep the interpass temperature below 150 deg. c. 4. Do not weld continuously at one place, spread out the heat. 5. Keep the heat input low, dont puddle at one place.
The above will avoid precipitation of manganese carbide and resulting hardenability.
There are two brands that we have used for welding on a shot blast cabinent, which is made of manganese plate. First, "STOODY" 1/8" Nicromang, Second, "STULTZ" 1/8" Manganese XL.
These were a couple SMAW rods used for repairs. John Wright
The Maintenance Welding Manual, published by ESAB, deals extensively with the applications you're talking about. I've got the Portuguese language edition of the manual, but surely there must be an English edition. Check with ESAB. According to the manual, for bucket teeth working with soils made up of fine grains, OK Selectrode 84.78 eletrodes should be used. For teeth working with rocky soils, OK Selectrode 83.58 eletrodes are the choice. Giovanni S. Crisi Sao Paulo - Brazil