1.Physical Properties -700 Mpa,, Yeild 370 Elongation 8%
Chemical -C 0.52-0.58 %,Si-.60 Max, Mn-1 Max, S -0.040 Max, P 0.040 Max
Cr-0.2 Max,
Ni- 0.30 Max
Mo-0.15 Max
Cu-0.25 Max
What electrode I should go for
The material is a medium carbon with minor alloy additions. I would approach it as a medium carbon steel, using sufficient preheat and I would use an undermatched low hydrogen filler metal if the joint is highly restrained.
Al