![](/mwf/attachments//avatars/4269-2369.jpg)
I'm trying to look up something on the wire and gas you are using, but I have struck out so far online
. Let us have all of the parameters to see if we can get you closer to what you need.
Solid Wire dia. = .045"
AWS Wire designation(ER70S-??) and classification(AWS A5.??)
Gas composition/blend?
Amperage?
Voltage?
cfh of gas flow?
travel angle?
push or drag?
If you can fill in a few answers to these questions, we should be able to get you in the ballpark as far as your parameters.
For instance: ESAB's .045" wire(ER70S-2) (AWS A5.18)has parameters for spray transfer suggested like this:
DCEP(electrode positive)
CFH rates of 25-45
260-340amps
25-30volts
300-500ipm(feed rate)
with optimum spray settings listed as:
300amps
27volts
350ipm