can some one give me some info on this  let me know
Parent - - By samh (**) Date 12-15-2007 01:03
5/32 BEAD AND HOT PASS AND 3/16 FILLER AND CAP. ON SA-200 190 AND 65 ON BEAD. WILL HAVE TO ADJUST UP OR DOWN 5 AND 75 ON HP. PUT AT LEAST A 1/8 GAP AND MAYBE MORE ON YOUR THROATS TO GET YOUR BEAD AND HOT PASS IN WITHOUT TRAPPING SLAG. 
Parent - By Leo27 (*) Date 12-15-2007 01:08
thanks sam h  will do so