![](/mwf/attachments//avatars/4269-2369.jpg)
If you are asking about the thickness ranges(since you mentioned 3mm to unlimited, I'm assuming you are), then look at AWS D1.1:2015, Table 4.11 "edit.." for
Welder Qualification(as Lawrence mentioned watch the data)
(1) Test on plate
Groove / 25mm or over ---> Qualified Dimensions / Nominal Plate, Pipe, or Tube Thickness Qualified / 3mm to Unlimited and Note d: Also Qualifies for welding any fillet or PJP weld size on any thickness of plate, pipe or tubing.
"edit".... for
WPS Qualification See Table 4.2
(1) Tests on Plate
25mm and over ---> Nominal Plate, Pipe or Tube Thickness Qualified / 3mm to Unlimited
and Notes c,d
Note c For square groove welds that are qualified without backgouging, the maximum thickness qualified shall be limited to the test thickness
Note d CJP groove weld qualification on any thickness shall qualify any size of fillet or PJP groove weld for any thickness (see 4.11.3)